J. Mater. Sci. Technol. ›› 2019, Vol. 35 ›› Issue (3): 231-238.DOI: 10.1016/j.jmst.2018.09.054
• Orginal Article • Next Articles
Guangrong Liab, Guanjun Yanga*()
Received:
2018-05-23
Revised:
2018-06-12
Accepted:
2018-06-19
Online:
2019-03-15
Published:
2019-01-18
Contact:
Yang Guanjun
Guangrong Li, Guanjun Yang. Understanding of degradation-resistant behavior of nanostructured thermal barrier coatings with bimodal structure[J]. J. Mater. Sci. Technol., 2019, 35(3): 231-238.
Fig. 1. Morphologies and size distributions of agglomerates and nanosized powders [45]: (A) morphology of agglomerates; (B) surface morphology of agglomerates with nanosized powders; (C) size distribution of agglomerates; (D) size distribution of nanosized primary particles (d0.1: 10% particles have diameters smaller than the value 53.7?μm; d0.5: 50% particles have diameters smaller than the value 79.9?μm; d0.9: 90% particles have diameters smaller than the value 152.4?μm).
Parameter | Value |
---|---|
Plasma arc voltage (V) | 60 |
Plasma arc current (A) | 650 |
Flow rate of primary gas (Ar) (L?min-1) | 50 |
Flow rate of secondary gas (H2) (L?min-1) | 7 |
Flow rate of powder feeding gas (N2) (L?min-1) | 4.5 |
Spray distance (mm) | 100 |
Torch traverse speed (mm?s-1) | 500 |
Table 1 Parameters used for plasma spraying.
Parameter | Value |
---|---|
Plasma arc voltage (V) | 60 |
Plasma arc current (A) | 650 |
Flow rate of primary gas (Ar) (L?min-1) | 50 |
Flow rate of secondary gas (H2) (L?min-1) | 7 |
Flow rate of powder feeding gas (N2) (L?min-1) | 4.5 |
Spray distance (mm) | 100 |
Torch traverse speed (mm?s-1) | 500 |
Fig. 2 shows the polished cross-sections of the samples after progressively increasing the thermal-exposure duration. At the as-deposited state, the conventional sample exhibits a typical lamellar structure with inter-splat pores and intra-splat cracks. In contrast, the nanostructured sample exhibits a bimodal structure, which implies that medium gray nanozones are surrounded by the lighter lamellar zones. Moreover, the lamellar zone in the nanostructured samples is similar to that in the conventional samples. Regarding the structural evolution of the conventional samples, the number of large-sized pores (approximate size of 5-15?μm) observed at the as-deposited state decreases distinctly during the thermal exposure. Regarding the structural evolution of the nanostructured samples, the contrast between the nanozone and lamellar zone is not as distinct as in the as-deposited state. This may be attributed to the sintering occurring in both lamellar zones and nanozones.
Fig. 3 shows the changes of the in-plane elastic modulus as a function of the thermal-exposure duration. Common phenomena can be observed for the conventional and nanostructured samples. The elastic modulus exhibits a significant increase, at macroscale and microscale. Moreover, the evolution exhibits an obvious non-linear trend. A very rapid increase occurs at initial short exposure durations, while a gradual increase could be observed at following long exposure durations. Therefore, the increment mainly occurs during the initial exposure. The comparison between the conventional and nanostructured samples reveals that the elastic moduli at the as-deposited states are comparable. However, the increments in the nanostructured samples are lower than those of the conventional samples. This suggests that the nanostructured samples, to some degree, can retard the sintering-induced stiffening.
Fig. 4 shows the changes in the thermal conductivity as a function of the thermal-exposure duration. A similarity between the mechanical and thermal properties could be observed; the evolution trends of the thermal conductivity are also non-linear. Therefore, the fast increase at initial short durations turns into a significantly slower increase at long exposure durations. The comparison between the conventional and the nanostructured samples reveals that the nanostructured samples exhibit a slightly lower thermal conductivity at the as-deposited state. Moreover, it is clear that the increase in the nanostructured samples is not as significant as that of the conventional ones after long durations. Therefore, the nanostructured coatings weaken the degradation of the thermal insulation during thermal exposure.
Fig. 6. Quasi in-situ healing behavior of an inter-splat pore at lamellar zones: (A) inter-splat pore at 0?h; (B) local region of inter-splat pore at 0?h; (C) local region of inter-splat pore after thermal exposure for 20?h.
|
[1] | Xiaoxiao Wei, Li Jin, Fenghua Wang, Jing Li, Nan Ye, Zhenyan Zhang, Jie Dong. High strength and ductility Mg-8Gd-3Y-0.5Zr alloy with bimodal structure and nano-precipitates [J]. J. Mater. Sci. Technol., 2020, 44(0): 19-23. |
[2] | Hansi Jiang, Xiaoguang Qiao, Chao Xu, Shigeharu Kamado, Kun Wu, Mingyi Zheng. Influence of size and distribution of W phase on strength and ductility of high strength Mg-5.1Zn-3.2Y-0.4Zr-0.4Ca alloy processed by indirect extrusion [J]. J. Mater. Sci. Technol., 2018, 34(2): 277-283. |
[3] | B. Saeedi,A. Sabour,A. Ebadi,A.M. Khoddami. Influence of the Thermal Barrier Coatings Design on the Oxidation Behavior [J]. J Mater Sci Technol, 2009, 25(04): 499-507. |
Viewed | ||||||
Full text |
|
|||||
Abstract |
|
|||||